Metallographic atlas
52 structures with morphology, formation conditions and identification notes. The chapter structure follows our metallography training course: common structures (15), cast iron (12), heat-treated 45 steel (10), hypereutectoid steel (4), quench & temper notes (5), surface treatment (6). Full Chinese notes are on the Chinese edition of this page.
Common microstructures
Ferrite, pearlite, martensite, sorbite, troostite, bainite, austenite — prepared on the ZMP-2000 automatic polisher
| # | Structure | Key identification |
|---|---|---|
| 1 | Polygonal ferrite (armco iron) | Equiaxed white grains, straight boundaries, ~120 deg triple points |
| 2 | Acicular & Widmanstatten ferrite | Needles growing from prior-austenite boundaries; sign of overheating |
| 3 | Network ferrite | Pro-eutectoid ferrite along prior-austenite grain boundaries |
| 4 | Lamellar pearlite | Alternating ferrite/cementite lamellae, fingerprint pattern at 500x |
| 5 | 索氏体(细片状珠光体) | |
| 6 | 屈氏体(极细珠光体) | |
| 7 | Spheroidised pearlite | Globular carbides in a ferrite matrix; spheroidise-annealed condition |
| 8 | Upper bainite | Feathery sheaves, carbides between ferrite laths; poor toughness |
| 9 | Lower bainite | Dark needles with fine carbides at 55-60 deg to the needle axis |
| 10 | Lath (low-carbon) martensite | Parallel lath packets, grey-white, dislocation substructure |
| 11 | Plate (high-carbon) martensite | Lens-shaped plates with midrib, micro-cracks common |
| 12 | Retained austenite | Bright untempered patches between martensite plates; dimensional instability |
| 13 | Widmanstatten structure | Aligned ferrite/cementite plates into the grain; rate per GB/T 13299 |
| 14 | Banded structure | Alternating ferrite/pearlite bands from segregation plus rolling |
| 15 | Non-metallic inclusions | Oxides, sulphides, silicates; rate per GB/T 10561 / ASTM E45 |
Cast iron structures
Pig iron, grey iron, ductile iron, compacted graphite iron — graphite form per GB/T 7216, nodularity per GB/T 9441
| # | Structure | Key identification |
|---|---|---|
| 16 | Eutectic white iron | Ledeburite: cellular pearlite + cementite, no graphite |
| 17 | Hypoeutectic pig iron | Primary austenite dendrites in a ledeburite matrix |
| 18 | Hypereutectic pig iron | Coarse primary cementite plates through ledeburite |
| 19 | Grey iron, type A graphite | Uniform random flakes, medium length; best mechanical properties |
| 20 | Grey iron, type B graphite | Rosette clusters, fine centre and coarse rim |
| 21 | Grey iron, type D graphite | Fine undercooled interdendritic flakes with ferrite |
| 22 | Ductile iron, ferritic | Nodular graphite in ferrite; bull-eye rims, best ductility |
| 23 | Ductile iron, ferritic-pearlitic | Mixed matrix, balanced strength and elongation |
| 24 | Ductile iron, pearlitic | Highest strength, lowest elongation; pearlite content per GB/T 9441 |
| 25 | Compacted graphite iron | Vermicular graphite, >=80% compacted; between grey and ductile iron |
| 26 | Malleable iron (black heart) | Temper carbon rosettes in ferrite after graphitising anneal |
| 27 | Phosphide eutectic | Angular steadite at grain boundaries; wear resistance up, toughness down |
Heat-treated 45 steel
One steel grade through every heat treatment: hot-rolled, normalised, annealed, quenched, tempered, under- and over-heated
| # | Structure | Key identification |
|---|---|---|
| 28 | 45 steel, as-hot-rolled | Ferrite + lamellar pearlite, often banded |
| 29 | 45 steel, normalised | Fine pearlite/sorbite with thin ferrite network; 170-210 HB |
| 30 | 45 steel, fully annealed | Coarse ferrite + pearlite, <=187 HB, good machinability |
| 31 | 45 steel, oil quenched | Incomplete hardening: martensite + troostite; low hardenability |
| 32 | 45 steel, water quenched | Lath + plate martensite, 55-58 HRC |
| 33 | Water quench + low temper (200 C) | Tempered martensite, dark needles, 52-56 HRC |
| 34 | Water quench + medium temper (400 C) | Tempered troostite; highest elastic limit, 40-45 HRC |
| 35 | Water quench + high temper (600 C) | Tempered sorbite; the classic quench-and-temper structure |
| 36 | 45 steel, 780 C water quench (underheated) | Blocky undissolved ferrite, soft spots - temperature too low |
| 37 | 45 steel, 1100 C water quench (overheated) | Coarse martensite needles spanning the prior grain; cracking risk |
Hypereutectoid steel
T8–T12 tool steel and GCr15 bearing steel: annealing, normalising, spheroidising, quench and temper
| # | Structure | Key identification |
|---|---|---|
| 38 | Hypereutectoid steel, annealed | Network cementite plus lamellar pearlite; network removed by normalising |
| 39 | Hypereutectoid steel, normalised | Fine sorbite, network broken up; standard pre-treatment for bearing steel |
| 40 | Hypereutectoid steel, spheroidise annealed | Uniform 0.5-1 um carbides, 187-217 HB, ready for machining |
| 41 | Hypereutectoid steel, quenched and tempered | Cryptocrystalline martensite + fine carbides + retained austenite |
Quench & temper notes
Reading ferrite morphology, lamellar and spheroidised pearlite, martensite and surface decarburisation
| # | Structure | Key identification |
|---|---|---|
| 42 | Morphology of ferrite | Equiaxed, acicular, network and banded - each points to a process cause |
| 43 | Lamellar pearlite in detail | Lamella spacing 0.15-0.45 um sets the strength level |
| 44 | Spheroidised pearlite in detail | Carbide size and uniformity drive machinability and cold forming |
| 45 | Reading martensite | Lath vs plate; needle length is direct evidence of overheating |
| 46 | Surface decarburisation | Full + partial decarburisation measured per GB/T 224 |
Surface treatment
Carburised, carbonitrided and nitrided cases plus full and partial decarburisation — case hardness on the HVT-1000A
| # | Structure | Key identification |
|---|---|---|
| 47 | Carburised and hardened case | Fine needle martensite + carbides + retained austenite; no carbide network |
| 48 | Carburised core | Lath martensite or bainite; excess ferrite means cooling too slow |
| 49 | Nitrided case | White compound layer 5-30 um plus diffusion zone; hardness gradient by micro-indentation |
| 50 | Carbonitrided case | Shallow (0.3-0.8 mm) but harder than carburised; porosity per GB/T 34807 |
| 51 | Full decarburisation | Columnar ferrite layer, no carbon left; reported separately |
| 52 | Partial decarburisation | Ferrite fraction decreasing inwards; total = full + partial |