मेटलोग्राफ़ी · कठोरता · यांत्रिकी · प्रकाशिकी — एक श्रृंखलामेटलोग्राफ़ी और परीक्षण
राष्ट्रीय हाई-टेकशंघाई एसएमई2 पेटेंट

Metallographic atlas

52 structures with morphology, formation conditions and identification notes. The chapter structure follows our metallography training course: common structures (15), cast iron (12), heat-treated 45 steel (10), hypereutectoid steel (4), quench & temper notes (5), surface treatment (6). Full Chinese notes are on the Chinese edition of this page.

CH.1

Common microstructures

Ferrite, pearlite, martensite, sorbite, troostite, bainite, austenite — prepared on the ZMP-2000 automatic polisher

#StructureKey identification
1Polygonal ferrite (armco iron)Equiaxed white grains, straight boundaries, ~120 deg triple points
2Acicular & Widmanstatten ferriteNeedles growing from prior-austenite boundaries; sign of overheating
3Network ferritePro-eutectoid ferrite along prior-austenite grain boundaries
4Lamellar pearliteAlternating ferrite/cementite lamellae, fingerprint pattern at 500x
5索氏体(细片状珠光体)
6屈氏体(极细珠光体)
7Spheroidised pearliteGlobular carbides in a ferrite matrix; spheroidise-annealed condition
8Upper bainiteFeathery sheaves, carbides between ferrite laths; poor toughness
9Lower bainiteDark needles with fine carbides at 55-60 deg to the needle axis
10Lath (low-carbon) martensiteParallel lath packets, grey-white, dislocation substructure
11Plate (high-carbon) martensiteLens-shaped plates with midrib, micro-cracks common
12Retained austeniteBright untempered patches between martensite plates; dimensional instability
13Widmanstatten structureAligned ferrite/cementite plates into the grain; rate per GB/T 13299
14Banded structureAlternating ferrite/pearlite bands from segregation plus rolling
15Non-metallic inclusionsOxides, sulphides, silicates; rate per GB/T 10561 / ASTM E45
CH.2

Cast iron structures

Pig iron, grey iron, ductile iron, compacted graphite iron — graphite form per GB/T 7216, nodularity per GB/T 9441

#StructureKey identification
16Eutectic white ironLedeburite: cellular pearlite + cementite, no graphite
17Hypoeutectic pig ironPrimary austenite dendrites in a ledeburite matrix
18Hypereutectic pig ironCoarse primary cementite plates through ledeburite
19Grey iron, type A graphiteUniform random flakes, medium length; best mechanical properties
20Grey iron, type B graphiteRosette clusters, fine centre and coarse rim
21Grey iron, type D graphiteFine undercooled interdendritic flakes with ferrite
22Ductile iron, ferriticNodular graphite in ferrite; bull-eye rims, best ductility
23Ductile iron, ferritic-pearliticMixed matrix, balanced strength and elongation
24Ductile iron, pearliticHighest strength, lowest elongation; pearlite content per GB/T 9441
25Compacted graphite ironVermicular graphite, >=80% compacted; between grey and ductile iron
26Malleable iron (black heart)Temper carbon rosettes in ferrite after graphitising anneal
27Phosphide eutecticAngular steadite at grain boundaries; wear resistance up, toughness down
CH.3

Heat-treated 45 steel

One steel grade through every heat treatment: hot-rolled, normalised, annealed, quenched, tempered, under- and over-heated

#StructureKey identification
2845 steel, as-hot-rolledFerrite + lamellar pearlite, often banded
2945 steel, normalisedFine pearlite/sorbite with thin ferrite network; 170-210 HB
3045 steel, fully annealedCoarse ferrite + pearlite, <=187 HB, good machinability
3145 steel, oil quenchedIncomplete hardening: martensite + troostite; low hardenability
3245 steel, water quenchedLath + plate martensite, 55-58 HRC
33Water quench + low temper (200 C)Tempered martensite, dark needles, 52-56 HRC
34Water quench + medium temper (400 C)Tempered troostite; highest elastic limit, 40-45 HRC
35Water quench + high temper (600 C)Tempered sorbite; the classic quench-and-temper structure
3645 steel, 780 C water quench (underheated)Blocky undissolved ferrite, soft spots - temperature too low
3745 steel, 1100 C water quench (overheated)Coarse martensite needles spanning the prior grain; cracking risk
CH.4

Hypereutectoid steel

T8–T12 tool steel and GCr15 bearing steel: annealing, normalising, spheroidising, quench and temper

#StructureKey identification
38Hypereutectoid steel, annealedNetwork cementite plus lamellar pearlite; network removed by normalising
39Hypereutectoid steel, normalisedFine sorbite, network broken up; standard pre-treatment for bearing steel
40Hypereutectoid steel, spheroidise annealedUniform 0.5-1 um carbides, 187-217 HB, ready for machining
41Hypereutectoid steel, quenched and temperedCryptocrystalline martensite + fine carbides + retained austenite
CH.5

Quench & temper notes

Reading ferrite morphology, lamellar and spheroidised pearlite, martensite and surface decarburisation

#StructureKey identification
42Morphology of ferriteEquiaxed, acicular, network and banded - each points to a process cause
43Lamellar pearlite in detailLamella spacing 0.15-0.45 um sets the strength level
44Spheroidised pearlite in detailCarbide size and uniformity drive machinability and cold forming
45Reading martensiteLath vs plate; needle length is direct evidence of overheating
46Surface decarburisationFull + partial decarburisation measured per GB/T 224
CH.6

Surface treatment

Carburised, carbonitrided and nitrided cases plus full and partial decarburisation — case hardness on the HVT-1000A

#StructureKey identification
47Carburised and hardened caseFine needle martensite + carbides + retained austenite; no carbide network
48Carburised coreLath martensite or bainite; excess ferrite means cooling too slow
49Nitrided caseWhite compound layer 5-30 um plus diffusion zone; hardness gradient by micro-indentation
50Carbonitrided caseShallow (0.3-0.8 mm) but harder than carburised; porosity per GB/T 34807
51Full decarburisationColumnar ferrite layer, no carbon left; reported separately
52Partial decarburisationFerrite fraction decreasing inwards; total = full + partial
तुलना ट्रे 0/4