Metallography · hardness · mechanics · optics — one chainMetallography & testing
National High-TechShanghai SME2 Patents

检测方法库:26 个项目的原理、步骤与误差

客户真正要判断的是「这个项目怎么测、按哪个标准判、哪里容易测错」。这一页把每个方法拆到原理公式、操作顺序、常见误差与依据标准,再落到在售机型;需要算具体数值的,直接去「原理与计算器」。

Hardness testing

Rockwell hardness

Measurement principle

A preliminary load F0 is applied, then the major load is added to reach the total load. After the major load is removed, the residual depth increase h is read in 0.002 mm units: HR = N − h/0.002. HRA/HRC use a 120° diamond cone (N=100); HRB uses a 1.5875 mm ball (N=130).

Where it applies

Hardened and tempered parts, finished parts after carburizing and quenching; the first choice for batch sampling — 5 seconds per part with an acceptable indentation.

Standard

GB/T 230.1ISO 6508-1ASTM E18

Procedure

  1. 1Pick the scale: HRA or superficial HR15N for thin and case-hardened parts, HRC for hardened parts, HRB for annealed parts
  2. 2Specimen surface Ra ≤ 1.6 µm, flatness ≤ 0.02 mm, faces parallel, thickness at least 10× the indentation depth
  3. 3Keep centres ≥ 3d apart and ≥ 2.5d from the edge; average at least 3 points per part
  4. 4Check with a reference block each shift; re-calibrate if the error exceeds ±1.5 HRC

Common errors

  • Back-face damage on thin walls reads 2–5 HRC low — always support the back face
  • Testing directly on a curved surface: below 25 mm radius a correction is mandatory, otherwise readings run low

Matching models

Hardness testing

Vickers and micro-Vickers hardness

Measurement principle

A 136° square-based diamond pyramid is pressed in under load F, leaving a square indentation. Measure both diagonals d1, d2 and average them to d: HV = 0.1891 × F / d² (F in N, d in mm). Because the indentation is geometrically similar, values from 10 gf to 50 kgf are directly comparable — the basis of case-depth gradients.

Where it applies

Thin sheets, case-hardened and coated layers, weld HAZ, small parts and microstructural phases; with image measurement it becomes an automated gradient scan.

Standard

GB/T 4340.1ISO 6507-1ASTM E384

Procedure

  1. 1Choose the load from layer thickness: thickness ≥ 1.5× the diagonal; for a 0.1 mm case stay at or below 0.3 kgf
  2. 2Mount or clamp the specimen, surface Ra ≤ 0.4 µm, and measure before etching
  3. 3Indentation corners must be sharp; keep the diagonal measurement error within ±0.5%
  4. 4For gradients measure every 10–20 µm and plot HV against depth to determine the effective case

Common errors

  • Too high a load punches through the case and reads the core — case depth is badly underestimated
  • Measuring near an edge or mounting resin reads low — keep indentations ≥ 2.5d from any boundary

Matching models

Hardness testing

Brinell hardness

Measurement principle

A hardened steel or carbide ball is pressed in under load F for a specified dwell, then the indentation diameter d is measured: HBW = 0.102 × 2F / [πD(D − √(D² − d²))], where D is the ball diameter. The large indentation averages coarse microstructures well — ideal for castings and forgings.

Where it applies

Cast iron, cast steel, forgings, non-ferrous blanks and quenched-and-tempered parts; also for hardness uniformity checks and furnace-batch verification.

Standard

GB/T 231.1ISO 6506-1ASTM E10

Procedure

  1. 1Select ball and load from the F/D² ratio in GB/T 231.1: for steel, φ10 mm at 3000 kgf (30D²) for 10–15 s
  2. 2Specimen thickness ≥ 8× indentation depth, Ra ≤ 1.6 µm, no hammer marks on the back face
  3. 3Measure the diameter in two perpendicular directions with a reading microscope and average
  4. 4Centres ≥ 4d apart, ≥ 2.5d from edges; three points per part

Common errors

  • A diameter outside 0.24D–0.6D means load and material do not match — the result is invalid
  • An unchecked worn ball reads high — verify the ball diameter every 2000 tests or quarterly

Matching models

Metallographic preparation

Metallographic specimen preparation

Measurement principle

Cutting, mounting, grinding/polishing and etching have one goal: a surface free of deformation and scratches that shows the true microstructure. Cutting damages 50–200 µm deep, and every last micron must be removed by stepped grinding, or both structure and hardness are misread.

Where it applies

Incoming material inspection, heat-treatment validation, failure analysis, weld-joint rating, coating and case observation.

Standard

GB/T 13298ASTM E3GB/T 10561

Procedure

  1. 1Cut with a resinoid or diamond blade, feed rate matched to hardness; the smaller the cut the shallower the damage — precision cutters are mandatory for thin and case-hardened parts
  2. 2Mount with phenolic resin at 150 °C/15 MPa for hot mounting, cold mounting for temperature-sensitive parts; add copper gauze or conductive resin to protect edges
  3. 3Grind 400 → 800 → 1200 → 2000 grit, each step until the previous scratches are gone, rotating 90° between steps; finish with 1 µm diamond polish
  4. 4Etch with 2–4% nital for 3–8 s on carbon steel, aqua regia or electrolytic etching for stainless; rinse and dry immediately

Common errors

  • Under-polishing leaves a deformed layer that smears grains together and biases grain-size ratings finer
  • Rounded mounting edges make case-depth measurement near the edge unreliable — use edge-protection mounting

Matching models

Metallography & case

Case-depth determination

Measurement principle

Effective case depth has two criteria: the hardness method measures from the surface to where hardness falls to a specified limit (550 HV1 is common for carburized and quenched parts); the metallographic method uses the visible structural boundary. Results are comparable, but the hardness method is objective and is used for arbitration.

Where it applies

Case depth and gradient evaluation for carburizing, carbonitriding, nitriding, induction and laser hardening; a key acceptance item for gears, bearings and pins.

Standard

GB/T 9450GB/T 11354ISO 2639

Procedure

  1. 1Section perpendicular to the surface (no chamfer, no torch cutting), prepare per metallographic standards with edge protection
  2. 2Use 0.3–1 kgf micro-Vickers, one point every 10–20 µm from the surface, to at least 1.5× the expected depth
  3. 3Plot HV against depth and take the point where hardness reaches the limit (e.g. 550 HV1) as the effective depth
  4. 4Cross-check metallographically after etching; a large discrepancy points to a process issue

Common errors

  • Overheated sectioning creates a re-hardened white layer and inflates the reading by 10–30 µm
  • Overlapping indentations interfere when closer than 3d and read high

Matching models

Mechanical testing

Tensile testing (yield & UTS)

Measurement principle

A standard specimen is pulled at a controlled rate while force and extension are recorded: yield strength ReH/ReL is read from the yield plateau or the 0.2% proof stress, Rm is the maximum force divided by the original cross-section, and elongation A comes from the final gauge length.

Where it applies

Strength and ductility of plate, bar, wire, weld joints, fasteners and plastics; the baseline test for incoming verification and process comparison.

Standard

GB/T 228.1ISO 6892-1ASTM E8

Procedure

  1. 1Machine a proportional specimen per GB/T 228.1 (L0 = 5.65√S0 is common); no scratches on the grip section or fillets
  2. 2Measure the original cross-section (average of three readings) and align the grips to avoid bending
  3. 3Keep the elastic rate ≤ 0.00025/s, raise to ≤ 0.008/s after yield, and remove the extensometer after yield
  4. 4Reassemble the halves to measure the final gauge length and neck diameter, then compute A and reduction of area Z

Common errors

  • Slipping raises the apparent yield point and damages the grip section — use hydraulic wedge grips
  • Testing too fast inflates both yield and UTS and widens scatter within a batch

Matching models

Environment & reliability

Neutral salt spray test

Measurement principle

A 5% NaCl solution is atomised at 35 °C and settles on the specimen at a 1–2 mL/80 cm²/h deposition rate; corrosion resistance is judged by time to first corrosion or by corroded area. Salt spray is an accelerated test — extrapolating to service life requires the specific material and coating system, never a linear conversion.

Where it applies

Corrosion resistance and process comparison for plating, coatings, anodised layers, fasteners and automotive or offshore parts.

Standard

GB/T 10125ISO 9227ASTM B117

Procedure

  1. 1Prepare 5% NaCl at pH 6.5–7.2 (adjust with HCl or NaOH), density 1.029–1.036
  2. 2Place specimens at the standard angle, not touching or shading each other; scribe to substrate per GB/T 10125 when required
  3. 3Spray continuously and inspect every 24 h; record time to first rust and corrosion grade at 24/48/96/240 h
  4. 4Rate per GB/T 6461 and archive photos taken under standard lighting

Common errors

  • Uncleaned oil films prevent corrosion and inflate the result
  • Not measuring deposition rate hides a blocked nozzle — the real exposure is far below nominal

Matching models

Dimensional metrology

Autocollimation (small angles & straightness)

Measurement principle

Collimated light leaves the objective, returns from a plane mirror and images on the focal plane. When the mirror tilts by θ the image shifts Δ = 2f·tanθ, so θ = Δ/(2f). With f the focal length, read on a reticle or CCD, a 300 mm autocollimator resolves angles of the order of 0.1″.

Where it applies

Guideway straightness, surface-plate flatness, rotary-table indexing error, parallelism of optical components and prism angles; also for flatness checks on large flats.

Standard

GB/T 11336GB/T 1958ISO 12781

Procedure

  1. 1Align the autocollimator to the mirror so the return image sits within ±10″ of the reticle centre
  2. 2Distribute stations evenly along the measured length (200–500 mm spacing is common) and record each reading
  3. 3Compute straightness by cumulative or least-squares fitting, reporting the maximum deviation and its position
  4. 4Let the environment stabilise for at least 2 h; keep air currents and vibration out of the beam path

Common errors

  • A poor mirror adds its own error one-to-one — use a λ/10 flat
  • Over long spans, earth curvature and thermal gradients matter — apply corrections beyond 10 m

Matching models

Metallography & case

Grain-size rating

Measurement principle

Grain size G is defined by the number of grains per unit area: N = 2^(G−1), where N is grains per square inch at 100×. Comparison charts, planimetric and intercept methods are used; the intercept method is preferred for arbitration.

Where it applies

Incoming grain-size acceptance, inherent grain size of carburizing steels, HAZ coarsening assessment, recrystallised grain checks in copper and aluminium alloys.

Standard

GB/T 6394ASTM E112ISO 643

Procedure

  1. 1Prepare and etch per GB/T 6394 until grain boundaries are clear; use picric acid or electrolytic etching for prior-austenite boundaries
  2. 2Take at least five random fields at 100×, avoiding edges and inclusion clusters
  3. 3Intercept method: draw test lines of known length L, count intercepts P, average intercept l = L/(P·M), then convert to G
  4. 4Have two operators rate independently; a difference above 0.5 grade calls for re-preparation

Common errors

  • Over-etching widens boundaries, inflating intercept counts and biasing the rating finer
  • A 5% magnification error alone shifts G by about 0.15 grade

Matching models

Cleanliness & NDT

Component cleanliness testing

Measurement principle

The part is rinsed at a specified pressure and flow, particles are collected on a filter membrane, counted by size class and weighed. Results are expressed as particles per unit area plus maximum particle size, which map directly to wear and jamming risk after assembly.

Where it applies

Cleanliness acceptance and process-improvement comparison for automotive parts, hydraulics, bearings, fuel injection, semiconductors and medical devices.

Standard

ISO 16232VDA 19.1GB/T 38214

Procedure

  1. 1Choose the extraction method per ISO 16232 (pressure rinse, ultrasonic, shake), then fix the fluid and duration
  2. 2Run a blank first: background particles on the membrane and in the fluid must be below 10% of the limit
  3. 3Filter, then count by class with a microscope or automatic counter (5–15, 15–25, 25–50, >50 µm)
  4. 4Dry and weigh for total mass, then normalise to mg/m² using the rinsed area

Common errors

  • Uncontrolled background air can multiply results — work in a clean bench
  • Weighing alone misses a few large particles that weigh little but do the damage — always report size distribution

Matching models

Metallographic preparation

Sectioning for metallography

Measurement principle

A thin abrasive wheel or diamond wire cuts the specimen under copious coolant, keeping sampling damage to a minimum. The cut zone contains a plastically deformed layer and a heat-affected layer whose depth depends on wheel speed, feed rate and cooling; grinding must remove it completely before the microstructure represents the parent metal.

Where it applies

The first step for every metallographic specimen: castings, forgings, welds, case-hardened parts, coatings, sheet, wire and small parts. Cut quality decides how long grinding takes and whether edge retention succeeds.

Standard

GB/T 13298ASTM E3ISO 4967

Procedure

  1. 1Choose the wheel by material: resin or sintered diamond for hardened steel and carbide, coarse grit with higher coolant flow for aluminium and copper
  2. 2Keep wheel speed at 25–45 m/s and feed at 1–3 mm/min; use the low end for thin walls and coatings, and cut perpendicular to the plane to be examined
  3. 3Clamp close to the cut and support long parts at both ends to avoid edge break-out; aim the coolant directly at the cut
  4. 4Mark orientation and position (rolling direction, surface, core) right after cutting and record the sampling sketch; leave enough allowance for the damaged layer

Common errors

  • Feeding too fast or cooling too little leaves blue temper colours and a re-tempered layer, so hardness reads low
  • Grinding with the side of the wheel bevels the surface; after mounting the edge is rounded and its microstructure is lost

Matching models

Metallographic preparation

Specimen mounting

Measurement principle

Irregular, small, thin or edge-critical specimens are encapsulated in a thermosetting resin under heat and pressure, or in a cold-mounting resin cured at room temperature. Mounting provides handling size, protects edges, fills porosity and makes resin and specimen wear at the same rate.

Where it applies

Small parts, sheet, wire, coating and case cross-sections, decarburised and plated specimens where the edge must survive; also used to standardise size for automated grinding and hardness mapping.

Standard

GB/T 13298ASTM E3ISO 19700

Procedure

  1. 1Hot mounting: 130–150 °C, 20–30 MPa, 5–10 min dwell; phenolic resin suits routine steel specimens
  2. 2Cold mounting: mix epoxy and hardener in ratio, de-air by vacuum or stirring, cure 4–8 h at room temperature; first choice for heat-sensitive materials and coatings
  3. 3Place the face to be examined downwards and support slender specimens to prevent tilting; keep height variation within 1 mm per batch
  4. 4Mark the number and orientation after demoulding and chamfer the resin edge by 0.5 mm to avoid edge rounding during grinding

Common errors

  • A large hardness gap between resin and specimen makes the resin wear faster and the specimen stand proud, producing a step at the edge
  • Trapped air in cold mounting collapses during polishing and looks like porosity or inclusions

Matching models

Metallographic preparation

Grinding and polishing

Measurement principle

Successively finer papers and cloths remove the cutting damage, each step erasing the scratches of the previous one until a mirror surface free of deformation remains. The rules are: rotate 90° between steps, allow enough time, reduce force with grit, and check under the microscope that earlier scratches are gone.

Where it applies

All metallographic specimens; edge-sensitive cases such as coatings, case layers and decarburisation need soft cloths, low force, short times and good mounting.

Standard

GB/T 13298ASTM E3ISO 19700

Procedure

  1. 1Rough grinding: 180 or 240 grit, 20–30 N, 300 rpm, until cut marks disappear and the face is flat
  2. 2Step through 400, 800, 1200 and 2000 grit, rotating 90° each time and dropping to 10–15 N
  3. 3Polish with 3 µm then 1 µm diamond on a soft cloth, low force and short time; use 0.05 µm silica for soft metals such as aluminium and copper
  4. 4Check at 100× after each step: earlier scratches must be gone, otherwise go back one step

Common errors

  • Skipping a step hides coarse scratches under polish; after etching they appear as artefacts
  • Excess force or time pulls out hard phases, rounds edges and drags graphite or inclusions into false pits

Matching models

Metallographic preparation

Etching and microstructure revelation

Measurement principle

In a suitable etchant, grain boundaries and phases dissolve selectively because of potential differences, creating relief and tint that reveal grains, pearlite, martensite and carbides under the microscope. Steels use 2–4% nital; stainless steels aqua regia or electrolytic etching; aluminium alloys Keller reagent.

Where it applies

Grain size rating, decarburisation and case interpretation, weld microstructure, heat-treatment verification and failure analysis; etch depth directly changes the rating.

Standard

GB/T 13298ASTM E407GB/T 6394

Procedure

  1. 1Polish to a scratch-free mirror, rinse with alcohol and dry before etching so no water film dilutes the etchant
  2. 2Swab or immerse for 5–15 s, checking under the microscope and stopping as soon as the structure appears
  3. 3Rinse immediately, dehydrate in alcohol and dry with cool air; never wipe, wiping destroys the etched surface
  4. 4Record etchant, time and temperature; comparative specimens must be etched identically or grain size is not comparable

Common errors

  • Over-etching widens boundaries and blurs pearlite lamellae, biasing grain size upward
  • Under-etching leaves only scratches and polish pits, easily mistaken for a fine structure

Matching models

Metallographic preparation

Decarburisation depth

Measurement principle

At high temperature surface carbon is burnt off, leaving a fully decarburised ferrite layer and a partially decarburised transition zone. Metallography measures it on a cross-section at 100× until the structure matches the core; microhardness traverses from the surface and uses the depth where hardness falls to a specified value.

Where it applies

Surface quality control for spring, bearing, tool steels, fasteners and quenched-tempered parts; decarburisation cuts fatigue life and is routine in fracture analysis.

Standard

GB/T 224GB/T 3098.1ISO 898-1

Procedure

  1. 1Cut perpendicular to the surface, mount to protect the edge and polish without edge rounding
  2. 2Etch lightly in 2–4% nital and scan from surface to core at 100×, recording the fully and partially decarburised boundaries
  3. 3For arbitration use microhardness: 0.05–0.1 kgf every 0.05 mm, judged to GB/T 3098.1 or GB/T 224
  4. 4Measure at least three positions and take the maximum; on threads measure the root, never the crest

Common errors

  • Rounding the edge during cutting or polishing removes the layer and produces a false zero
  • Over-etching lowers contrast and hides the partial zone boundary, biasing depth low

Matching models

Metallographic preparation

Non-metallic inclusion rating

Measurement principle

Oxides, sulphides, silicates and globular inclusions differ in reflectivity from the polished matrix and appear grey, black or pale. GB/T 10561 (ASTM E45) classes them as A sulphide, B alumina, C silicate and D globular, grading each by length or diameter and count in the worst field.

Where it applies

Cleanliness assessment for bearing, gear, spring and pipeline steels; inclusions are the main source of contact fatigue and cracks and a basis for steelmaking improvement.

Standard

GB/T 10561ASTM E45ISO 4967

Procedure

  1. 1Sample to GB/T 10561: longitudinal section, at least 200 mm², away from the decarburised surface
  2. 2Examine in the polished state without etching; scan the whole area at 100× and record maximum length and count per class
  3. 3Grade against the standard charts or image analysis software, rating thin and heavy series separately and taking the worst
  4. 4Confirm the type by EDS when needed so morphology alone does not mislead

Common errors

  • Over-polishing drags inclusions out into pits, overestimating count and length
  • Rating after etching is invalid because the matrix obscures inclusion boundaries

Matching models

Metallographic preparation

Coating thickness by cross-section

Measurement principle

Cut the coated part perpendicular to the surface, mount to protect the edge, polish and measure the coating thickness directly under the microscope. Unlike magnetic or eddy-current gauges it also shows uniformity, bonding, porosity and cracks, making it the arbitration method.

Where it applies

Electroplating, electroless plating, thermal spray, PVD/CVD, aluminising and chromising, oxide and paint layers; sprayed and diffused layers of 100–500 µm need low-magnification measurement with marked positions.

Standard

GB/T 6462ISO 1463ASTM B487

Procedure

  1. 1Cut perpendicular, cold mount to avoid heat-induced cracking and polish at low force to protect the edge
  2. 2Observe unetched; if the interface is unclear etch 2–3 s or use dark field for contrast
  3. 3Measure five evenly spaced points, record min, max and mean, and state magnification and scale
  4. 4For bond strength, combine with thermal shock or bend tests and observe interface cracking

Common errors

  • A tilted cut magnifies thickness by 1/cosθ; 10° already reads 1.5% high
  • Edge rounding makes thin coatings under 10 µm almost unmeasurable

Matching models

Mechanical testing

Charpy impact test

Measurement principle

A notched bar is supported as a simple beam and broken by a single swing of a pendulum; the energy absorbed is reported as KV2 or KU2 in joules. The notch concentrates stress, making the test very sensitive to toughness, ductile-brittle transition and metallurgical defects.

Where it applies

Toughness and transition assessment for pressure-vessel, pipeline, ship and low-temperature steels; also for weld HAZ, castings and heat-treatment comparison.

Standard

GB/T 229ISO 148-1ASTM E23

Procedure

  1. 1Machine 10×10×55 mm specimens to GB/T 229 with a 2 mm deep notch of 0.25 mm root radius, notch axis normal to the rolling direction
  2. 2Soak at test temperature (at least 20 min in liquid media) and break within 5 s of removal
  3. 3Choose a pendulum so the absorbed energy falls between 10% and 80% of range; test three specimens per condition and at least six temperatures for a transition curve
  4. 4Record shear-fibre percentage and lateral expansion, and photograph the fracture surface

Common errors

  • A specimen that is not soaked through reads high and underestimates low-temperature brittleness
  • Machining marks at the notch root raise stress concentration and cut energy by 10–30%

Matching models

Mechanical testing

Bend test

Measurement principle

The specimen rests on two rollers and a former applies three-point bending; after bending to a specified angle the tension surface is inspected for cracks. Compared with tension, bending is more sensitive to surface defects and welds because the maximum tensile stress sits exactly at the surface.

Where it applies

Weld procedure qualification, cold-bend ductility of plate and sections, coating adhesion, casting and forging surface quality, and repeated bending of wire and sheet.

Standard

GB/T 232ISO 7438ASTM E290

Procedure

  1. 1Take full-thickness specimens, remove weld reinforcement and backing, and round the edges by 1–2 mm
  2. 2Set the roller span to 4t ± 0.2t and choose the former diameter from the standard or specification
  3. 3Load slowly and continuously below 0.1 rad/s to the specified angle, often 180° or 120°
  4. 4Inspect the tension surface at 10× and reject if crack length exceeds the limit

Common errors

  • Unrounded edges crack first and are mistaken for low ductility
  • Bending too fast raises surface temperature and adds impact effects, giving inconsistent results

Matching models

Mechanical testing

Fatigue testing

Measurement principle

Under cyclic loading, damage accumulates well below the tensile strength until fracture. The S-N curve relates stress amplitude to life, and the fatigue limit is the highest stress surviving 10⁷ cycles. The test needs constant amplitude, accurate alignment and a stable high-frequency loading system.

Where it applies

Life assessment for springs, shafts, connecting rods, bolts, blades and welded structures; also before/after surface treatments such as shot peening, carburising and rolling.

Standard

GB/T 3075ISO 1099ASTM E466

Procedure

  1. 1Machine plain or notched specimens to standard with Ra ≤ 0.4 µm so machining marks do not start cracks
  2. 2Check alignment after clamping; eccentricity must stay below 5% of stress amplitude or scatter explodes
  3. 3Run a step test from high to low stress with one or two specimens per level; take 10⁶–10⁷ cycles as the conditional limit
  4. 4Record crack origin and beach marks to identify surface defects, inclusions or corrosion pits

Common errors

  • Misalignment turns a nominal 300 MPa into 400 MPa locally and shortens life by an order of magnitude
  • Too high a frequency self-heats the specimen and lengthens life, especially for polymers and aluminium

Matching models

Dimensional metrology

Straightness and parallelism by autocollimation

Measurement principle

An autocollimator projects a parallel beam that returns from a mirror; tilting the mirror by θ shifts the image by 2θ. Moving a mirror on a bridge along the surface gives an angle profile that is integrated into a straightness error in µm/m or over the full length.

Where it applies

Machine guideways, surface plates, granite tables and long parts with tight straightness; also parallelism, squareness and flatness. Photoelectric autocollimators with 10–50 m range suit shop-floor use.

Standard

GB/T 11336ISO 230-1JJG 202

Procedure

  1. 1Set the instrument at the same height as the surface, roughly aligned, and warm up 15 min until readings stabilise
  2. 2Move the bridge in equal steps (100 or 200 mm), read after stabilising and average the forward and return runs
  3. 3Convert angle to height difference: Δh = L × tanθ ≈ L × θ in radians, then accumulate to obtain the profile
  4. 4Evaluate straightness by the minimum-zone method and report both full-length and per-metre errors

Common errors

  • A temperature gradient from sunlight or lamps drifts readings by 2–3 arcsec within half an hour
  • A bridge that does not match the support span includes its own sag, especially over long spans

Matching models

Dimensional metrology

Small angle and rotary indexing measurement

Measurement principle

Autocollimator sensitivity comes from focal length and reticle: typical resolution 0.1 arcsec over ±600 arcsec. With a flat mirror on the table or prism, rotating by a nominal angle and reading the residual gives the indexing error.

Where it applies

Calibration of rotary tables, indexing heads, polygons and optical benches; also pitch and yaw of precision guideways and angle calibration of collimators and lenses.

Standard

JJG 202GB/T 17421.1ISO 230-1

Procedure

  1. 1Mount the mirror face square to the axis within ±30 arcsec so the reading stays in range
  2. 2Index the table in 15° or 30° steps, read in both directions and average to remove backlash
  3. 3Close the traverse on the first reading and adjust to obtain the indexing error curve
  4. 4Judge to JJG or the acceptance specification, reporting maximum indexing error and repeatability

Common errors

  • A loose mirror sags after 90° and its mount distortion is read as indexing error
  • Measuring one direction only folds backlash into the result and forward/reverse runs disagree

Matching models

Microscopy

Bright-field and dark-field observation

Measurement principle

Bright field: light passes through the objective onto the specimen and the reflected light forms the image, with contrast from reflectivity and etch relief. Dark field: an annular stop makes the illumination oblique so only scattered light enters, making pores, cracks, inclusions and boundaries glow.

Where it applies

Bright field for routine microstructure, grain size and decarburisation; dark field for crack paths, porosity, inclusions and polish damage; also useful for coating cross-sections.

Standard

GB/T 13298ASTM E3ISO 643

Procedure

  1. 1Set Köhler illumination first: image the filament at the aperture stop and open the field stop just beyond the field of view
  2. 2In bright field close the aperture stop to 70–80% of the objective NA to balance contrast and resolution
  3. 3Switch to a low-power objective before inserting the dark-field stop and raise brightness gradually
  4. 4Capture bright-field and dark-field images of the same field and annotate magnification and scale

Common errors

  • Polish pits look like inclusions in dark field; rack focus or rotate the stage to tell them apart
  • A wide aperture stop gives brightness but kills contrast, blurring fine pearlite

Matching models

Microscopy

Image measurement and grain size

Measurement principle

Calibrated optics and camera convert pixels to micrometres so length, area, angle and phase fraction can be measured. Grain size to GB/T 6394 uses comparison or intercept: count boundary intersections on a line of known length and derive G from the mean intercept.

Where it applies

Quantitative grain size, phase fraction, coating thickness, decarburisation depth, inclusion size and spacing, porosity; also crack length and spacing in failure analysis.

Standard

GB/T 6394ASTM E112ISO 643

Procedure

  1. 1Calibrate with a stage micrometer for every magnification and record µm per pixel; recalibrate after changing objectives
  2. 2Illuminate evenly without clipping; adjust the aperture rather than stretching contrast in software
  3. 3For grain size use intercepts on at least five lines in three fields with no fewer than 50 intersections
  4. 4Report uncertainty and sample count; a single field is not a valid basis for rating

Common errors

  • Measuring without calibration differs by 10–30% between objectives
  • Rating after over-etching widens boundaries and raises the grain-size number

Matching models

Metallographic preparation

Weld cross-section examination

Measurement principle

Cut across the weld, mount, polish and etch, then examine bead shape, fusion line, HAZ width, porosity, slag and cracks at low and high magnification. The HAZ sees different thermal cycles and forms coarse-grain and partially recrystallised zones that are weak links for hardness and toughness.

Where it applies

Weld procedure qualification, pressure vessel and pipeline joints, dissimilar steel welds, hardfacing and HAZ hardness gradients; also weld cracking analysis.

Standard

GB/T 226NB/T 47014ISO 17639

Procedure

  1. 1Take a transverse section to NB/T 47014 or GB/T 226 covering parent metal, HAZ and weld metal
  2. 2Use 10–50× for macro shape, lack of fusion and porosity; etch in 4% nital or a weld-specific etchant
  3. 3At 200–500× measure HAZ width, grain coarsening and precipitates
  4. 4Run a microhardness traverse normal to the fusion line (0.2–0.5 kgf every 0.2 mm) to find soft or hard zones

Common errors

  • Cutting only the weld centre misses lack of fusion and cold cracks at the fusion line, which are usual fracture origins
  • Over-etching blurs the HAZ so its width and hardness profile cannot be matched to structure

Matching models

Non-destructive testing

X-ray radiography

Measurement principle

X-rays attenuate with density and thickness; defects such as porosity, slag and lack of penetration attenuate less and appear as density differences on film or a digital detector. Detectable size is about 1–2% of section thickness, and volumetric defects are easier to find than planar cracks.

Where it applies

Casting porosity and shrinkage, weld lack of penetration and cracks, internal structure of electronics and batteries; also composite delamination and assembly misalignment.

Standard

GB/T 3323ISO 17636ASTM E94

Procedure

  1. 1Choose kV and exposure by thickness: about 100–120 kV per 10 mm of steel, lower kV for thin parts to raise contrast
  2. 2Set focus distance from F ≥ 2 × source size × thickness to limit geometric unsharpness
  3. 3Place an image quality indicator to standard and verify the index after exposure
  4. 4For digital imaging average multiple frames to cut noise, then classify defect type, size and level to standard

Common errors

  • A crack parallel to the beam barely changes attenuation and is invisible; change the angle
  • Unshielded scatter greys the film and drowns small defects in noise