原理与计算:19 个现场可算的公式

硬度公式、压痕几何、切割线速度、自准直角度、渗层测点载荷、拉伸与冲击、晶粒度、显微分辨率,再加上渗碳层深度插值、球化率、努氏硬度、陶瓷断裂韧性与侵蚀剂配比——这些量每天都要算,却常在 Excel 里手工套。这一页给出公式与单位约定,改一个数就出结果,并标明什么时候不能用。

Vickers hardness from the diagonals

HV = 0.1891 × F / d²
Vickers hardness—
Mean diagonal—

Enter both diagonals; the mean is used. F in N, d in mm. 1 kgf = 9.80665 N.

Valid only when the indentation is clearly measurable; a 1% diagonal error shifts HV by about 2%.

Brinell hardness from the indentation diameter

HBW = 0.102 × 2F / [πD(D − √(D² − d²))]
Brinell hardness—
Ratio d/D—

d/D must fall between 0.24 and 0.60; outside this the load does not match the material.

3000 kgf equals 29420 N. Never use Brinell on case-hardened or thin parts — the indentation exceeds the layer thickness.

Hardness conversion: HV → approximate HRC

HRC ≈ 100 − 15400 / HV
Rockwell HRC (approx.)—
Brinell HBW (approx.)—

For rough comparison on the same material without test conditions only; acceptance and arbitration must use measured hardness.

Conversion curves vary with material and heat treatment; GB/T 1172 and ASTM E140 do not agree exactly.

Indentation depth and minimum thickness

t = d / (2·tan68°) ≈ d / 4.95
Indentation depth t—
Minimum thickness (10t)—

GB/T 4340.1 requires thickness of at least 1.5× the diagonal; in practice 10t is safer.

Specimens thinner than the minimum show an anvil effect and read systematically high.

Metallographic cutting: wheel speed and feed

v = π × D × n / 60000
Surface speed—
Range check—

Resinoid blades typically run at 25–45 m/s: keep to the low end for carbide and ceramics, the high end for soft materials such as aluminium and copper.

Too high a speed burns the specimen (re-hardened white layer); too low is slow and deepens the deformed layer.

Autocollimator: image shift to angle

θ = Δ / (2f)
Angle (arcsec ″)—
Angle (µrad)—

1″ = 4.848 µrad. Over long spans take stations every 200–500 mm, then compute straightness cumulatively.

A poor mirror adds its error one-to-one — use a λ/10 flat.

Case measurement: maximum test force

dmax = t / 1.5;Fmax = HV × dmax² / 0.1891
Maximum diagonal—
Recommended max. force—
Nearest scale—

The diagonal must not exceed 2/3 of the case depth, or the indenter reads the core instead.

This is an engineering rule of thumb; formal judgement still uses the HV–depth curve and the limit hardness.

Uncertainty of repeated measurements

u = s / √n;U = 2u
Mean—
Std. deviation s—
Standard uncertainty u—
Expanded uncertainty U (k=2)—

Covers the Type A (repeatability) component only; a full evaluation adds Type B terms such as reference block and instrument error.

With n below 5 the deviation itself is unreliable — take more readings or use the range method.

Tensile: elongation and reduction of area

A = (Lu − L0)/L0 × 100%;Z = (S0 − Su)/S0 × 100%
Elongation A—
Reduction of area Z—

标距按 5.65√S0 选取;断后标距须把两段断口对齐后测量,不能直接拼。

延伸率对试样尺寸与标距敏感,不同标距的数据不能直接比较。

Impact: absorbed energy and toughness

aKU = KV2 / S0
Impact toughness aKU—

10×10×55 mm 标准试样的缺口截面为 0.8 cm²;6.7 mm 厚的小尺寸试样按实测截面计算。

冲击功是整根试样吸收的能量,与试样尺寸强相关,不能跨尺寸换算。

Grain size from intercept counts

G = −3.2877 + 6.6439 × lg(N_L)
Grain size number G—
Mean intercept—

N_L 用截点法在至少 5 条测线上统计;G 允许半级,报「G = 8.0」或「8 级」均可。

比较法评级更快但主观;有争议时以截点法为准。

Microscope: resolution and depth of field

d = 0.61λ / NA;DOF ≈ λ / (2NA²)
Limit of resolution—
Depth of field—

白光取 550 nm;NA 越大分辨率越高但景深越浅,高倍观察粗糙断口时尤其明显。

这是光学极限,实际可分辨尺寸还受摄像头像素与照明方式限制。

Brinell: test force from ball diameter

F = 0.102 × k × D²(k = 30 / 10 / 5)
Test force F—
Equivalent kgf—

压痕直径 d 应落在 0.24D–0.60D;超出说明载荷与材料不匹配,需换标尺。

布氏压痕深,薄件与渗层件不得使用;仲裁时按产品标准指定的 F/D² 组合。

Indent layout: spacing and minimum size

间距 ≥ 3d,边距 ≥ 2.5d,厚度 ≥ 10t
Min. centre spacing—
Min. edge distance—
Min. specimen width—
Min. specimen thickness—

硬度换算表与验收判定都假定压痕互不干扰;间距不足会让读数系统性偏低。

焊接接头与渗层梯度测量时,间距还要满足「每点代表一个区域」的要求。

Case depth: 550 HV1 effective depth

DC = d1 + (HV1 − 550)(d2 − d1) / (HV1 − HV2)
Effective case depth DC—

在硬度–深度曲线两端各取一点做线性插值,求极限硬度 550HV1 所在深度;两点越靠近 550,插值越准。

d1 处硬度须高于 550、d2 处低于 550;渗氮件与表面淬火件的极限硬度值按产品标准取(常见 550HV1 或 50HRC)。

Ductile iron: nodularity rating

球化率 = Σ(nᵢ × fᵢ) / N × 100%(f = 1 / 0.8 / 0.6 / 0.3 / 0)
Nodularity—
Grade (GB/T 9441)—

至少数 200 个石墨球;视场数不少于 3 个。系数:球形 1.0、团状 0.8、团絮状 0.6、蠕虫状 0.3、片状 0。

蠕虫状与片状石墨混入会快速拉低球化率;报告须写明放大倍数与视场数。

Knoop hardness from the long diagonal

HK = 1.451 × F / d²
努氏硬度 HK—

努氏压痕浅而长,适合渗层、镀层与极薄件;只测长对角线,短对角线约为其 1/7。

HK 与 HV 数值不可直接比较;努氏压头对试样表面粗糙度更敏感,抛光到 1μm 以下再测。

Ceramic fracture toughness by indentation

KIC = 0.16 × H × √a × (c/a)^(−1.5)
Fracture toughness KIC—
c/a 判定—

H 由 HV × 9.807 换算为 MPa;a 取压痕对角线一半,c 为压痕中心到裂纹尖端。c/a ≥ 2 属中位裂纹体系,公式才成立。

压痕法是半经验方法,与 SEPB/SEVNB 法可能差 10–20%;不同文献的经验系数在 0.1–0.2 之间,报告须注明所用公式与系数。

Etchant mixing: nital

V(HNO₃) = C × V;V(乙醇) = V − V(HNO₃)
Conc. nitric acid volume—
Absolute ethanol volume—

2–4% 硝酸酒精是钢铁金相最常用侵蚀剂;配好后密封避光保存,变黄失效不可再用。

必须把硝酸缓缓加入乙醇并不断摇动,严禁反向操作;腐蚀性液体操作请在通风橱内进行。

Unit conventions and common conversions

QuantityConversion
Force1 kgf = 9.80665 N;1 N = 0.10197 kgf
Hardness scalesHV 0.1 / 0.3 / 1 / 5 = 0.9807 / 2.942 / 9.807 / 49.03 N
Angle1° = 60′ = 3600″;1″ = 4.848 μrad
Length1 μm = 0.001 mm;1 mil = 25.4 μm
Surface speedv(m/s) = π × D(mm) × n(r/min) / 60000

These calculators support engineering estimates and selection checks; they do not replace the test procedures defined by standards. Reported results must come from laboratory measurement.